Galvanizing practice

Designing steel for galvanizing: vents, drains and steel choice

Many galvanizing problems are decided on the drawing board. A checklist for fabricators and their customers.

Galvanizing dips the whole piece in liquids: degreaser, acid, rinse, flux and then molten zinc at 450 °C. Every liquid must reach every surface and drain out again, and every closed space must let air out. Design for that and most problems disappear.

Vent and drain

  • Every closed or boxed section needs vent and drain holes at diagonally opposite corners. A sealed hollow section can burst in the kettle: trapped air and moisture expand violently. Never send sealed hollow parts.
  • Cut corners off gussets and stiffeners so zinc can flow past them.
  • Leave pipes and tubes open at both ends.
  • Avoid pockets and recesses that hold liquid.

Joints and overlaps

  • Seal-weld overlapping surfaces, or leave a gap wide enough to clean and drain; small gaps trap acid that weeps out later as rust stains.
  • Blast or grind weld slag; use a welding process that leaves little slag.
  • Keep threads and holes in mind: clearances for zinc on bolts and nuts.

Size and shape

  • Check the piece fits the kettle, with room around it: by our rule, kettle inside length = largest article + 100 mm, width + 100 mm, depth + 200 mm. Bigger pieces may be double-dipped, at a cost in finish.
  • Avoid joining very thin and very thick parts in one piece; they heat at different rates and can distort.
  • Make symmetrical sections where possible; asymmetric ones tend to bow.
  • Provide lifting points or holes for hanging.

Choose the steel

Specify steel chemistry suited to galvanizing: silicon at or below about 0.03 %, or about 0.15 to 0.25 %, with low phosphorus. Mixing steels of different chemistry in one assembly gives different coating thickness and colour on each part.

Surface condition

Avoid paint, oil-based marking and stickers on surfaces to be galvanized, and use removable or water-based markers. Remove silicone and anti-spatter sprays. Castings need blasting to remove sand.