Die angle, reduction per pass and why wire breaks
Most breaks on a drawing machine are designed in: by the die sequence, the die angle and the lubrication. The few numbers that decide whether wire draws cleanly.
Wire drawing pulls rod through a die smaller than itself. The die squeezes the wire down, the block pulls it through, and the wire comes out thinner, longer, stronger and harder. Every pass is a balance: the pull needed to draw the wire must stay well below the strength of the wire that has already been drawn, or the wire breaks just after the die.
Reduction per pass
Reduction is measured on area. A pass from 5.5 mm to 4.82 mm takes 23 per cent off the cross-section. Larger reductions need fewer dies but a higher drawing stress in each one. In practice, low carbon wire is usually drawn at up to about 25 per cent per pass, medium and high carbon at about 20 per cent, and stainless and alloy grades at less. The last die usually takes a lighter reduction, for close size control and a good surface.
| Material | Typical largest reduction per pass |
|---|---|
| Low carbon steel | About 25 % |
| Medium carbon steel | About 22 % |
| High carbon steel | About 20 % |
| Stainless steel | About 18 % |
Die angle and the delta factor
The die's approach angle and the reduction together decide how the metal flows. Engineers combine them in one number, the delta factor: delta = (angle / reduction) × (1 + √(1 − reduction))², with the half-angle in radians and the reduction as a fraction. For a 6° half-angle and a 25 per cent reduction, delta is about 1.5; for 8° and 20 per cent it is about 2.5.
- A low delta means a long contact zone: more friction, more heat and more die wear.
- A high delta means a short, steep contact zone: more internal shear, and above about 3 a risk of central bursts, the cup-and-cone breaks that start inside the wire.
- Most die sequences aim for a delta between about 1 and 3. Lighter reductions need smaller die angles to stay in that range.
Drawing stress against wire strength
The pull at each die divided by the area of the wire leaving it is the drawing stress. It must stay well below the tensile strength of that wire: most die sequences keep it under about 60 to 65 per cent. Above that, small variations from a worn die, a dry spot in the soap box or a weld are enough to break the wire. The SHIVAS wire calculator works out the stress for every die and flags a pass that runs too close.
The usual causes of breaks
- A pass with too much reduction for its die angle, or a die angle worn open.
- Poor lubrication: soap box empty, wrong soap for the speed, or rod not coated after descaling.
- Scale or rust left on the rod by poor descaling or pickling.
- Weak butt welds that were not annealed or trimmed.
- Wire running hot: high carbon wire that gets too hot between blocks becomes brittle. Block and die cooling matter.
- Misalignment between die and block, which bends the wire as it leaves the die.