Dipping practice: immersion, time and withdrawal
The same steel, the same zinc, two operators, two results. What happens in the minutes the work spends in the kettle, and how to make it repeatable.
Before dipping
- Bath at working temperature, usually about 445 to 455 °C, measured in the bath, not only at the wall.
- Surface skimmed clear where the work will go in and come out.
- Work hung so air can escape and zinc can drain, at an angle, with vents and drain holes open.
Immersion
Lower the work at a steady speed. Too slow, and the part already in the zinc reacts longer than the rest, so the coating is uneven; flux on the upper part also has longer to burn. Too fast, and zinc splashes and air is trapped. Watch the bath: it boils as the flux burns off and the steel heats up.
Time in the zinc
The work is ready when the boiling stops: the steel has reached bath temperature and the alloy layers have formed. Thin steel takes a minute or two; heavy sections longer. Leaving work in beyond that adds alloy layer, especially on reactive steel, and costs zinc.
Withdrawal
Withdrawal speed decides how much pure zinc stays on the work and how smooth it is. A slower, steady withdrawal lets zinc drain back into the bath and gives a thinner, smoother coat; a fast one leaves runs and drips. Skim the surface just before the work comes out, so it leaves through clean zinc.
| Variable | Effect if too low | Effect if too high |
|---|---|---|
| Bath temperature | Poor drainage, runs, lumps | Thicker alloy on reactive steel; faster kettle wear |
| Immersion speed | Uneven coating along the part | Splashing; trapped air; dross stirred up |
| Time in zinc | Incomplete reaction, bare or thin areas | Extra coating; brittle coatings on reactive steel |
| Withdrawal speed | Slow throughput | Runs, drips, extra zinc |
Make it repeatable
Record bath temperature, immersion and withdrawal times for each type of work, and use crane speed control so the operator can repeat them. Automatic control of the dip cycle takes the variation out of it.