Coating defects

Dull grey, thick and flaking coatings

Why some steel comes out heavy and grey, when that is only a matter of looks, and when it turns into a real problem.

A bright, spangled coating is mostly pure zinc over thin alloy layers. A dull grey coating is alloy right through to the surface. Both protect the steel; protection depends on thickness, not shine. But very thick alloy coatings are brittle, and they cost the galvanizer zinc.

The causes

CauseWhat happens
Reactive steel: silicon about 0.03 to 0.12 % or above 0.25 %, and phosphorusThe alloy layers keep growing instead of slowing down; the coating comes out thick and grey
Long immersionReactive steel keeps growing coating for as long as it stays in the zinc
High bath temperatureFaster reaction, thicker alloy
Heavy sections that cool slowlyThe reaction carries on after the work leaves the bath and turns the pure zinc to alloy
Thick welds and castingsDifferent chemistry from the parent steel

Flaking and peeling

Very thick coatings, often above about 250 µm, can crack and flake at edges and corners when the work is knocked or bent. This is a real defect: the steel is exposed where the coating comes off.

What the galvanizer can do

  • Keep immersion only as long as it takes for the reaction to settle.
  • Run the bath at the lower end of the normal range, around 445 °C, for reactive work.
  • Use bath alloying: small nickel additions calm reactive steel in the Sandelin range.
  • Quench heavy sections promptly after withdrawal, where the steel and the customer allow it, to stop the reaction.
  • Handle and stack thick-coated work with care.

What the customer can do

Specify steel for galvanizing: silicon at or below about 0.03 %, or between about 0.15 and 0.25 %, with phosphorus low. Ask the mill for certificates. Where looks matter, say so in the order, and agree what finish is acceptable.