Sizing a galvanizing kettle: the 100 mm rule and the ten-times check
The kettle is the most expensive item in the plant and the hardest to change later. How we size it from your largest article, and the checks we make on tonnage.
Every galvanizing plant is designed around one decision: the size of the zinc kettle. It fixes the longest article you can galvanize in one dip, the throughput the plant can hold, the zinc you have to buy before the first load, and the fuel you will burn every day to keep that zinc molten. It is also the item that is most expensive and slowest to change once the furnace is built around it.
The SHIVAS rule: article plus 100 mm
We size the kettle from the largest article you want to galvanize in one dip, measured as length (L), width (B) and height as dipped (H). Every extra centimetre of kettle is zinc to buy, heat to supply and surface to lose heat from, so we keep the margins tight:
| Kettle dimension | Rule | Example: article 6.0 × 1.2 × 1.5 m |
|---|---|---|
| Inside length | L + 100 mm | 6.10 m |
| Inside width | B + 100 mm | 1.30 m |
| Depth | H + 100 mm of zinc below the article + 100 mm empty at the top | 1.70 m |
The 100 mm of zinc below the work keeps it clear of the kettle floor, where dross settles. The 100 mm left empty at the top is the freeboard: it stops zinc washing over the flange when a load goes in and the level rises. The zinc fill is therefore the kettle depth minus 100 mm.
Length: your longest article
Inside length is set by the longest article you want to dip in one go. A plant for 12 m poles gets a kettle of 12.1 m; a solar purlin plant working with 6 m members can use a much shorter one, and saves zinc and fuel every day as a result.
Articles longer than the kettle can be galvanized by double dipping, one end at a time. It works, but the overlap gets a double coating, the process is slower and the risk of distortion rises. If long articles are a regular part of your work, size the kettle for them.
Width and depth
Width follows the widest article or bundle plus 100 mm. Depth is the tallest article as dipped plus 200 mm: 100 mm of zinc below the work and 100 mm of freeboard above the zinc. Deeper kettles hold more zinc and keep temperature better, but every extra 10 cm on a 7.5 m kettle is about 6 t more zinc to buy, so depth is set by the work, not by habit.
The ten-times rule
When you dip a load of cold steel, it takes heat out of the zinc. If the zinc mass is too small, the bath temperature drops, the coating quality suffers and the dip cycle slows while the furnace catches up. A long-standing rule of thumb is that the kettle should hold at least ten times the steel you want to galvanize per hour.
| Hourly throughput | Minimum zinc in kettle | Typical kettle (L × W × D) |
|---|---|---|
| 1 t/h | 10 t | 6 × 1.2 × 1.5 m |
| 2 t/h | 20 t | 7.5 × 1.2 × 2 m (holds ≈ 110 t) |
| 4 t/h | 40 t | Set by article size; usually far above 40 t |
In practice, kettles sized for long structural articles usually hold far more than ten times their throughput, and the rule only bites for short, small-article kettles and spin plants. It is still the first check we make.
Throughput: dips per hour
A kettle's output is the steel per dip times the dips per hour. A dip cycle of 10 to 15 minutes, including lowering, immersion, withdrawal and skimming, gives four to six dips an hour. Load per dip is limited by the crane, the jig and how much steel the bath can absorb at once. Monthly tonnage then follows from working hours and how much of that time the kettle actually works.
Heat follows size
The furnace has to supply the heat taken by the steel and the replacement zinc, plus the losses from the bath surface and walls, which continue around the clock. A large kettle running at low throughput spends most of its fuel just staying hot. That is why idle-hour covers, good insulation and planning production into fewer, fuller shifts all reduce fuel per tonne.