Two of the most common complaints have nothing to do with how well the steel was cleaned: zinc that did not drain, and fresh zinc that stayed wet.

Runs, drips and spikes

Zinc that does not drain freely freezes on the work as runs, drips and spikes along the lower edges. Besides looking poor, spikes can cut hands and stop parts fitting together.

  • Withdraw at a steady, controlled speed; pulling out too fast leaves more zinc to drain.
  • Keep the bath at its working temperature; cold zinc does not drain.
  • Hang the work at an angle so zinc runs to one corner and off.
  • Vibrate or tap the work over the kettle, and wipe spikes while the zinc is still liquid.
  • Ask for drain holes at the corners of closed and boxed sections, as the design guides for galvanizing show.
  • Spin small parts in a basket to throw off excess zinc.

White rust (wet storage stain)

Fresh zinc is very reactive. If galvanized work stays wet, with little air, for example stacked tightly in the rain or packed while still damp, a white or grey powder forms on the surface. This is zinc hydroxide and zinc carbonate, usually called white rust or wet storage stain.

  • Passivate after quenching; a conversion film greatly slows white rust in the first weeks.
  • Store work off the ground, stacked with spacers and sloped so water runs off.
  • Keep it under cover or ventilated; do not wrap wet work in plastic.
  • Dispatch dry.
How badWhat to do
Light filmUsually weathers away in service; brush off if needed
Heavy white depositBrush off and check coating thickness
Dark grey under the deposit, thickness below specificationRepair or re-galvanize

Rust weeping from joints

Brown streaks running from overlapping plates or bolted joints weeks after galvanizing come from pickling acid trapped in the gap, which slowly weeps out. Seal-weld overlaps, or leave a gap wide enough to clean and drain.