Is your kettle wearing out? Wall checks and warning signs
Kettles rarely fail without warning. Wall temperatures, dross and fuel trends, wall bulge and the leak pits: what to log every day, and when to plan the change.
Zinc dissolves the kettle wall all the time. An evenly heated kettle loses steel slowly and lasts for years; a kettle with a hot zone loses it fast in one place. A kettle that fails in service lets molten zinc into the furnace, stops the plant for weeks and puts people at risk. A planned change costs a fraction of that, and the signs that it is due are there to be read.
How a kettle wears
- General thinning. All the wetted wall loses steel at a slow rate set by the zinc temperature and the steel of the kettle.
- Local thinning at hot spots. Where a burner jet or hot gas strikes, the wall runs hotter and dissolves much faster. Above about 480 °C the attack speeds up sharply.
- Thinning behind dross. Dross insulates the wall it sits against; if that part of the wall is heated, it runs hot.
- Bulging. Hot steel under the weight of the zinc creeps slowly outwards, and thinner walls bulge faster.
What to log every day
- Wall temperatures in every zone, with the zinc temperature. Note the highest wall reading and the spread between zones. A zone that runs hotter than the others for weeks is wearing faster.
- Firing: burner load or fuel used, and fuel per tonne. A rise with no change in production points at the lining, the casing or the burners.
- Zinc level and zinc added. A level that falls faster than production explains is a leak until proved otherwise.
- Dross removed, each week and per tonne. A rise with no change in the work or the flux can mean the wall is dissolving faster.
- Leak pit thermocouples. A rising reading means zinc in the pit.
At each shutdown, or when the kettle is emptied
- Measure the wall thickness with an ultrasonic gauge on a fixed grid of points, closer together in the zones that run hot. The same points every time make the trend clear.
- Measure the bulge of each long wall from a straight line at several heights.
- Inspect the welds, the corners and the rim.
- Inspect the furnace lining, baffles and burner blocks while the furnace is open.
Working out the remaining life
For example, a wall that started at 50 mm and measures 44 mm at its thinnest point after three years is losing 2 mm a year there. If the kettle maker's retirement thickness is 30 mm, there are about seven years left at that rate. If the same point read 47 mm a year earlier, the rate has risen to 3 mm a year and less than five years are left. The trend matters more than any single reading.
Warning signs
| Sign | What it can mean | Action |
|---|---|---|
| One wall zone runs hotter than the others | Burner jet, baffle or lining problem; local wear | Check burner alignment, baffles and lining; limit firing in that zone |
| Dross per tonne rising | More iron from the flux, the steel or the wall | Check flux iron first, then the wall temperatures |
| Fuel per tonne rising | Lining damage, casing leaks, burner tuning | Inspect lining and casing; tune the burners |
| Zinc level falling without explanation | Leak | Check the leak pits at once; get the emergency plan ready |
| Leak pit thermocouple rising | Zinc in the leak pit | Stop firing that zone; follow the emergency plan |
| Bulge larger than at the last check | Creep of a hot or thin wall | Measure, lower the heat flux, plan the change |
| Zinc seen in the furnace or the flue | Wall breach | Emergency stop |
Plan the change
- Order the new kettle well before the old one reaches its retirement thickness. Kettle steel and fabrication take time.
- Plan the zinc transfer: pumping the zinc into moulds or a holding vessel takes equipment and time, and a zinc pump sized for the job makes it safer and quicker.
- Reline and inspect the furnace while the kettle is out, and check the burners, baffles and thermocouples. See installing a new kettle.
- Write the emergency plan for a kettle leak before you need it: who stops what, where the zinc goes, and how water is kept away.